Inclusions in aluminum: causes and prevention
An inclusion is non-metallic material trapped inside the aluminum: an oxide film, a hard particle or a remnant of refractory or flux. This page explains where they come from and how they are reduced. It is general metallurgy: your plant’s values (temperatures, times, doses) follow the plant’s procedure.
What they are
Section titled “What they are”- Oxide films and bifilms. The most common. Liquid aluminum is covered at once by an oxide skin. If the surface breaks and folds inward (turbulence, splashing, a high drop), that skin enters the metal. When it folds it becomes double, with one dry face against another: that is a bifilm.
- Spinels (MgAl₂O₄). Aluminum and magnesium oxides. They appear mostly in alloys with magnesium and when the metal is held in the furnace for a long time.
- Carbides (Al₄C₃). Fine particles of aluminum carbide.
- Borides and TiB₂ agglomerates. They come from the grain refiner. Its particles are useful when loose, but they can clump into clusters.
- Refractory or flux particles. Pieces of the lining of the furnace, the ladle or the launder, and remnants of flux salts that did not come out with the dross.
How each one looks in the fracture: Inclusion classification.
Where they come from
Section titled “Where they come from”- The charge. Dirty, oily, wet or oxidized scrap brings in oxide and moisture from the start.
- Metal handling. Each transfer, each pour with a high drop and each splash folds new oxide inward.
- The tools. A wet, cold or uncoated tool brings in oxide and moisture, and can shed particles.
- The refractory. A worn or damaged lining sheds particles.
- The treatment. Poorly removed flux or a poorly dissolved refiner leaves remnants.
- Time and temperature. Holding the metal for a long time or very hot makes the oxides grow (and, in alloys with magnesium, the spinels).
Why they matter
Section titled “Why they matter”- Fatigue. An inclusion is a weak point: the part tends to crack there under repeated loads.
- Leaks. In parts that must be pressure-tight, an oxide film can open a path for the fluid.
- Porosity. Bifilms open easily: hydrogen and shrinkage inflate them and turn them into pores. Less oxide usually means less porosity.
- Machining. Hard particles (spinels, carbides, borides, refractory) wear the tool and leave marks on the machined surface.
That is why customers like VW ask for evidence of cleanliness before accepting the material.
How the K-mold detects them
Section titled “How the K-mold detects them”The K-mold produces a thin notched plate. It is broken into several pieces and the fracture faces are examined. The fracture tends to run through the weak points, so the inclusions are left exposed on the face.
- A sound face has a gray granular texture. An oxide film, a particle or a bifilm interrupts that texture.
- In the VW test 3 samples are taken: the first 2 preheat the mold and are discarded, and the third is analyzed. Zap calculates density and index and, separately, the informative K (K = S / n) face by face.
- Not everything dark is an inclusion: marker ink, pores, shrinkage, shadows and reflections are artifacts. See the Is it an inclusion or an artifact? table.
The step-by-step test is in Do the K-mold test. The internal procedure is ITPR-33: check the current ITPR-33.
Good practices to reduce them
Section titled “Good practices to reduce them”No single practice solves the problem: inclusions are prevented along the whole chain. The specific values follow the plant’s procedure.
- Clean, dry charge. No oil, moisture, paint or dirt. Moisture also brings in hydrogen.
- Transfers and pouring without turbulence. Low drop height, continuous flow and no splashing. Each fold of the surface brings in new oxide.
- Careful skimming. Remove the dross calmly, without stirring the skim into the bath.
- Dry, preheated, coated tools. A wet or cold tool brings in moisture and oxide.
- Flux treatment. It helps separate the oxides from the metal and carry them to the dross. Remove the dross well afterwards.
- Rotary degassing. Besides removing hydrogen, the bubbles drag oxides to the surface.
- Settling time after treatment. Let the particles float up or settle before pouring.
- Ceramic foam filtration. It traps films and particles in the last step before the mold.
- Temperature control. Overheating forms more oxide and makes the metal absorb more hydrogen.
- Refractory maintenance. Check and repair the lining before it sheds particles.
- Sampling discipline. Always take the sample the same way: same spot, same ladle, preheated mold. Otherwise the test measures how the sample was taken and not the metal.
See also